白色彩涂板出現(xiàn)的質量問題?請聽佛山萬慶分享及分析

2022-11-26 17:17
原作者: 佛山萬慶物資 收藏 分享 邀請

彩涂板是冶金和化工相結合的表面處理工程的重要產(chǎn)品,彩涂板作為表面技術處理產(chǎn)品,其產(chǎn)品質量不僅僅局限于產(chǎn)品的理化性能(膜厚、光澤、柔韌性、耐反向沖擊性、耐溶劑性、耐腐蝕性、耐候性等),還包括彩涂板產(chǎn)品的 ...

      彩涂板是冶金和化工相結合的表面處理工程的重要產(chǎn)品,彩涂板作為表面技術處理產(chǎn)品,其產(chǎn)品質量不僅僅局限于產(chǎn)品的理化性能(膜厚、光澤、柔韌性、耐反向沖擊性、耐溶劑性、耐腐蝕性、耐候性等),還包括彩涂板產(chǎn)品的涂層表面質量。

      Color coating is an important product of metallurgical and chemical surface treatment engineering, color coating as a surface technology products, the product quality is not limited to the physical and chemical performance of the product (film thickness, luster, flexibility, reverse impact resistance, solvent resistance, corrosion resistance, weather resistance, etc.), also includes the coating surface quality of color coating products.

      1. 彎曲性不良

      特點:鋼材彎曲180度試驗時,加工部位的涂層發(fā)生龜裂及涂層剝離

      發(fā)生原因:

      1)、前處理的掌握量過多。

      2)、涂層厚度過厚。

      3)、過度烘烤。

      4)、下涂涂料同上涂涂料的制造廠家不同,或稀料的使用不當。

      1.Poor curvature

      Features: When the steel bending 180 degrees test, the coating of the processing site crack and coating stripping

      Causes:

      1)Too much mastery of pre-processing.

      2) The coating thickness is too thick.

      3) Excessive baking.

      4) The lower coating is different from the manufacturer of the upper paint, or the improper use of dilute materials.

      2.硬度不良

      特點:用制圖鉛筆用力在涂層表面劃一道,擦去后表面留下一道劃痕

      發(fā)生原因:

      1)爐溫低,涂層固化不充分。

      2)加熱條件不適當

      3)涂層厚度比規(guī)定的厚

      2. Poor hardness

      Features: Use a drawing pencil to scratch the coating surface, wipe off the rear surface and leave a scratch

      Causes:

      1) The furnace temperature is low, and the coating curing is not sufficient.

      2) Improper heating conditions

      3) The coating thickness is thicker than that specified

      3. 凸點

      特點:由于鋼帶受到外部的沖擊,板表面出現(xiàn)突出或凹陷,有的有一定的間距,有的沒有

      發(fā)生原因:

      1)涂裝時輥上有異物混入。

      2)薄板產(chǎn)品在捆扎時的扎痕。

      3)倒卷時受到外部沖擊。

      3. The convex point

      Features: because of the steel belt by the external impact, the plate surface appears prominent or depression, some have a certain spacing, some do not

      Causes:

      1)There are foreign matter on the roller during coating.

      2) Tie marks of sheet products during binding.

      3) Get external impact when inverted.

      4. 邊部氣泡

      特點:兩側沾有涂料,經(jīng)烘干,出現(xiàn)氣泡

      發(fā)生原因:原材有毛刺沾有涂料多,兩邊出現(xiàn)縫隙

      4.The convex point

      Features: because of the steel belt by the external impact, the plate surface appears prominent or depression, some have a certain spacing, some do not

      Causes:

      1) There are foreign matter on the roller during coating.

      2) Tie marks of thin plate products during binding.

      3) Get external impact when inverted.

      4)Side air bubbles Features: both sides are stained with coating, after drying, air bubbles appear Cause of occurrence: raw material has burr stained has paint much, both sides appear gap

      5.麻點

      特點:從外部混入的異物或灰塵在涂裝后部分或全部表面有米粒樣的突出發(fā)生原因:

      1)涂料中混入其它種類或其它公司的涂料。

      2)涂料中有異物混入引起。

      3)前處理過程中水洗不良。

      5. The hemp point

      Features: Foreign body or dust mixed from the outside highlights on some or all of the surface after coating

      Causes:

      1)Mix aint with other types or other company coatings.

      2) Mixed substances caused by foreign bodies in the paint. 3) Poor water washing during pretreatment.

      6.橘皮

      特點:已干燥的表面涂層象橘子皮一樣粗糙,不均勻

      發(fā)生原因:

      1)濕膜過厚。

      2)涂料的黏度較高時。

      6. Orange peel

      Features: The dried surface coating is as rough and uneven as the orange peel

      Causes:

      1)The wet film is too thick.

      2) When the viscosity of the coating is high.

      7.耐溶劑性能差

      特點:丁酮擦拭有點狀掉漆

      發(fā)生原因:

      1)烘烤溫度沒有達到要求

      2)涂料的固化有問題

      3)前處理清洗不干凈

      7. Poor solvent resistance performance

      Features: Butanone wipe a bit off the paint

      Causes:

      1) The baking temperature did not meet the requirements

      2) The curing of the coating is problematic

      3) The cleaning is not clean

      8.沖擊不合格

      特點:漆膜沖擊后,經(jīng)膠帶粘后部分或全部掉漆

      發(fā)生原因:

      1)前處理不佳

      2)檢查面漆固化溫度是否合理

      8.Inqualified impact

      Features: paint film impact, part or all of the paint

      Causes:

      1)Poor pre-processing

      2) Check whether the curing temperature of the surface paint is reasonable

      9.縮孔

      特點:漆膜不平整,局部露底

      發(fā)生原因:

      1) 鋼帶表面不潔凈

      2)底漆冷卻水不潔凈

      3)涂料粘度沒達到上機要求

      9. Shaft hole

      Features: the paint film is uneven, and the local dew base

      Causes:

      1)The steel strip surface is not clean

      2) The primer cooling water is unclean

      3) The coating viscosity does not meet the upper machine requirements

      10.漏涂

      特點:面漆未涂上

      發(fā)生原因:

      1)邊部面漆未涂上,基板板型不好或涂輥與大背輥間壓力不足。

      2)板面中間面漆未涂上,底漆冷卻后板面有水或其它異物。

      10.Leakage

      Features: Finish is not painted

      Causes:

      1The side finish paint is not painted, the substrate plate type is not good or the pressure between the coated roller and the large back roller is insufficient.

      2The middle finish of the plate is not coated, and there is water or other foreign matter after cooling the primer.

      11.色差

      特點:同標準板的顏色出現(xiàn)差異

      發(fā)生原因:

      1)


      路過

      雷人

      握手

      鮮花

      雞蛋
      推薦資訊
      精選資訊
      閱讀排行
      精選案例展示

      微信二維碼

      掃一掃Get更多資訊

      Powered by Discuz! X3.4© 2001-2013 Comsenz Inc.|網(wǎng)站地圖

      *本站部分網(wǎng)頁素材及相關資源來源互聯(lián)網(wǎng),如有侵權請速告知,我們將會在24小時內(nèi)刪除*,關于【廣告法】【極限詞】【違禁詞】聲明:請各位職業(yè)舉報人高抬貴手繞行本站或發(fā)現(xiàn)問題請直接與我們聯(lián)系。 自從2017年新廣告法發(fā)布起,本公司積極響應廣告法的規(guī)定,已經(jīng)每年全面盤查網(wǎng)站的【極限詞】【違禁詞】3到5遍,但因網(wǎng)站內(nèi)容繁多加之人員排查力度有限,可能造成網(wǎng)頁部分地方仍存在遺漏【極限詞】【違禁詞】的現(xiàn)象,如發(fā)現(xiàn)遺漏【極限詞】【違禁詞】請及時通知我們整改下,從現(xiàn)在開始本公司宣傳網(wǎng)頁存在的所有廣告法【極限詞】【違禁詞】全部作廢失效,本公司也不承擔此類問題產(chǎn)生的投訴理賠。懇請各位職業(yè)舉報人高抬貴手繞行本站或發(fā)現(xiàn)問題請直接與我們聯(lián)系,如直接投訴就以本說明為準處理!